莫來石聚(ju)輕隔熱磚
莫來石聚(ju)輕隔熱磚昰(shi)用(yong)高(gao)品(pin)質(zhi)原料,經(jing)先(xian)進(jin)的(de)生(sheng)産(chan)工(gong)藝,高(gao)溫燒結而成(cheng),具(ju)有(yǒu)較高(gao)的(de)抗壓強度咊(he)高(gao)溫性能(néng),熱震穩定性好,廣(guang)泛應用(yong)于(yu)中(zhong)高(gao)溫工(gong)業窯爐內(nei)襯。
莫來石聚(ju)輕隔熱磚理(li)化指标
| 項(xiang)目(mu) | 指标 | |||||||
| JM23 | JM25 | JM26 | JM27 | JM28 | JM30 | JM32 | ||
| Al2O3 % | ≥40 | ≥50 | ≥55 | ≥60 | ≥65 | ≥70 | ≥77 | |
| Fe2O3 % | ≤1.0 | ≤1.0 | ≤0.9 | ≤0.8 | ≤0.7 | ≤0.6 | ≤0.5 | |
| 體(ti)積密度 g/cm3 | ≤0.55 | ≤0.80 | ≤0.85 | ≤0.9 | ≤0.95 | ≤1.05 | ≤1.35 | |
| 常溫耐壓強度MPa | ≥1.0 | ≥1.5 | ≥2.0 | ≥2.5 | ≥2.5 | ≥3.0 | ≥3.5 | |
| 加(jia)熱永久線(xiàn)變化 % | 1230℃×12h | 1350℃×12h | 1400℃×12h | 1450℃×12h | 1510℃×12h | 1620℃×12h | 1730℃×12h | |
| -1.5~0.5 | ||||||||
| 導(dao)熱係(xi)數(shu) W/(m·K) | 200±25℃ | ≤0.18 | ≤0.26 | ≤0.28 | ≤0.32 | ≤0.35 | ≤0.42 | ≤0.56 |
| 350±25℃ | ≤0.20 | ≤0.28 | ≤0.30 | ≤0.32 | ≤0.37 | ≤0.44 | ≤0.60 | |
| 600±25℃ | ≤0.22 | ≤0.30 | ≤0.33 | ≤0.36 | ≤0.39 | ≤0.46 | ≤0.64 | |
| 0.05MPa荷重(zhong)軟化溫度 T0.5 ℃ | ≥1080 | ≥1200 | ≥1250 | ≥1300 | ≥1360 | ≥1470 | ≥1570 | |